Sample
Name
Pellet of PVP-coated Ag nano-particles mixed with BN
Date
2014-01-01
Thickness
1.0 $\pm$ 0.5 $mm$
Diameter
5.0 $mm$
Mass
0.023 $\pm$ 0.006 $g$
Temperature
293.0 $\pm$ 5.0 $K$
Temperature max
293.0 $K$
Type
ambient air
Fluid temperature
293.0 $K$
Fluid pressure
1.0 $bar$
Title
mixing and compressing of PVP-coated Ag nanoparticles with BN

Precursors

Matters

Produced sample

Sample
Pellet of PVP-coated Ag nano-particles mixed with BN (this sample)
Processing steps
Step Chronology Date Type Process Changes
#1 before layer formation mixing Mixed BN and nanoparticles manually in mortar during 15 min
#2 during layer formation pressure Pressed with a manual hydraulic press up to 1.5 tons during 1 min